PCB Prepreg Types: How PP Works, Resin Content, and Pressed Thickness Calculation
2025-02-13

PCB Prepreg Types: How PP Works, Resin Content, and Pressed Thickness Calculation

When discussing PCB prepreg, do 1080, 2116, and 7628 immediately come to mind?

These are common prepreg glass styles used in multilayer PCB manufacturing. However, knowing these numbers alone is not enough to determine the final pressed thickness.

The same glass style can be supplied with different resin contents. Even with the same prepreg combination, different inner-layer copper thicknesses and copper retention ratios can produce different dielectric thicknesses after lamination.

To understand how prepreg affects a multilayer PCB stack-up, we first need to understand what happens during lamination.

1. What Is Prepreg, and How Does It Bond PCB Layers Together?

Prepreg, often abbreviated as PP, consists of woven glass fabric impregnated with partially cured resin.

For common FR-4 materials, it can be described simply as:

Prepreg = glass fabric reinforcement + a partially cured epoxy resin system.

These two components serve different purposes:

  • Glass fabric provides reinforcement and dimensional support.
  • Resin flows during lamination, fills the spaces between copper features, and bonds adjacent layers together.

The resin in a core laminate is already cured. The resin in prepreg can still flow and undergo further curing. This is what allows prepreg to serve as the bonding material between PCB layers.

During lay-up, the manufacturer arranges the inner-layer cores, prepreg, and copper foil according to the stack-up design. Controlled heat, pressure, and vacuum are then applied to laminate the assembly.

Lamination does not melt the copper or the cores. It causes the prepreg resin to flow, fill, and finally cure.

PCB Prepreg Types: How PP Works

PCB Prepreg Types: How PP Works

2. What Happens to Prepreg During Lamination In PCB Manufacturing?

Stage 1: Softening

As the temperature rises, the resin softens and its viscosity decreases.

The resin becomes mobile, preparing it to fill the spaces between inner-layer copper features. The glass fabric remains in place as reinforcement.

Stage 2: Flow and Filling

An etched inner layer is not a flat, continuous copper surface. It contains retained copper traces and areas where copper has been removed.

Under suitable temperature and pressure conditions, the resin flows into these etched areas, surrounds the copper features, and bonds the layers. Vacuum helps remove trapped air and reduces the risk of bubbles and voids.

Therefore, prepreg resin must do more than simply bond two layers together. It must also provide enough material to fill the etched spaces.

Stage 3: Gelation

As the curing reaction progresses, the resin begins to gel. Its ability to flow decreases, and the layer structure starts to become fixed.

An important distinction is:

Loss of flow does not mean full cure.

Stage 4: Full Cure

The resin must remain at the specified actual board temperature for sufficient time to achieve the required cure.

After lamination, the prepreg becomes a cured, glass-reinforced dielectric layer that provides bonding, electrical insulation, and mechanical support.

The image illustrates softening above approximately 90°C, lower viscosity near 130°C, and reduced flow near 150°C for selected epoxy prepregs. These are illustrative temperatures. Actual processing windows depend on the resin system and heating profile, and the lamination cycle must follow the material supplier’s requirements.

3. What Do 1080, 2116, and 7628 Mean?

These numbers primarily identify glass fabric styles. They do not specify a fixed finished prepreg thickness or resin grade.

Different glass styles have different yarn and weave constructions. Among these common styles, 1080 is relatively thin, 2116 is intermediate, and 7628 is thicker.

However, a complete prepreg specification requires more than the glass style. It should also identify:

  • Material manufacturer and resin system;
  • Glass fabric style;
  • Resin content, or RC;
  • Number and combination of prepreg plies;
  • Expected pressed thickness in the intended stack-up.

Material suppliers also list glass construction, resin content, and thickness separately in their prepreg data. A glass style number alone does not fully define the material.

Therefore, “use 2116 prepreg” is not a complete stack-up specification.

2116 prepreg with 48% resin content cannot automatically be treated as having the same thickness as 2116 prepreg with 57% resin content.

4. Why Does Resin Content Affect Prepreg Thickness?

Resin content normally refers to the percentage of the prepreg’s total mass contributed by resin.

For example, an RC of 53% generally means that resin accounts for approximately 53% of the prepreg’s total mass. It does not mean that resin accounts for 53% of its finished thickness.

For the same glass style and resin system, higher resin content generally means more resin per unit area. Under comparable lamination conditions, this usually results in greater pressed thickness.

However, not all of that resin remains between opposing copper surfaces. Some fills the etched areas of the inner layers, and some may flow toward the panel edges.

Therefore:

Resin content affects the available resin volume, copper patterns affect the filling demand, and the lamination process affects the final resin distribution.

This is why “7628” alone cannot define a fixed thickness suitable for every PCB.

5. Reference Prepreg Types Pressed Thicknesses for Different Resin Contents

The following data is based on our lamination reference table. The pressed thickness column uses the average values from the original records.

All thicknesses are shown in mils, rounded to one decimal place.

1 mil = 0.0254 mm.

Prepreg Glass Style Resin Content (RC) Reference Pressed Thickness (mil) Reference Glass Fabric Thickness (mil)
1080 62% 2.8 2.1
1080 65% 3.1 2.1
1080 68% 3.3 2.1
2113 56% 4.0 3.1
2116 48% 4.4 3.7
2116 53% 5.1 3.7
2116 57% 5.7 3.7
7628 44% 7.6 7.1
7628 48% 8.6 7.1

For 2116 prepreg, increasing the resin content from 48% to 57% increases the reference pressed thickness from 4.4 mil to 5.7 mil. The 44% and 48% resin-content versions of 7628 also show a clear thickness difference.

These values are references for particular materials and lamination conditions. They are not universal specifications for every prepreg manufacturer or every copper pattern.

The actual stack-up must be confirmed using material data, copper thickness, copper retention, and the PCB manufacturer’s lamination experience.

6. Why Can the Same Prepreg Combination Produce Different Thicknesses?

One key reason is that resin must fill the spaces left by etched copper.

This brings us to copper retention:

Copper retention ratio = retained copper area ÷ total area of the region being evaluated.

For example:

  • A 10% copper retention ratio means approximately 90% of the copper area has been etched away.
  • A 95% copper retention ratio means only approximately 5% has been etched away.

With the same copper thickness, lower copper retention generally creates a greater resin filling demand.

In a simplified comparison, with other conditions held equal:

Greater filling demand generally leaves less prepreg thickness between opposing copper surfaces. Lower filling demand generally leaves a thickness closer to the original reference value.

Copper thickness also amplifies this effect. For the same etched area, 2 oz copper creates more space to fill than 1 oz copper.

7. How Can Finished Prepreg Thickness Be Estimated?

For an initial stack-up assessment, a simplified volume-balance calculation can help explain how copper retention affects pressed thickness.

In words:

Estimated thickness = prepreg reference thickness − equivalent etched-space thickness on the first side − equivalent etched-space thickness on the second side.

If both sides have the same copper thickness and copper retention ratio:

   H=H0-2t*(1-R)

All thickness values must use the same units.

Example: Two Plies of 7628 Prepreg with 2 oz Copper on Both Facing Surfaces

The illustration uses the following independent assumptions:

  • Reference thickness per prepreg ply: 0.180 mm;
  • Total reference thickness for two plies: 0.360 mm;
  • Copper thickness on each facing surface: approximately 0.070 mm.

The 0.180 mm value is used only for this illustrative calculation. It is a separate assumption from the 7.6 mil reference value in the previous table.

Item 10% Copper Retention on Both Sides 95% Copper Retention on Both Sides
Prepreg combination 2 plies of 7628 2 plies of 7628
Total reference prepreg thickness 14.2 mil 14.2 mil
Copper thickness on each facing surface 2.8 mil 2.8 mil
Estimated dielectric spacing 9.2 mil 13.9 mil

Displayed thicknesses are rounded to one decimal place. Calculations use the original, unrounded values.

The difference between these two estimates is:

  0.353-0.234=0.119 

That is approximately 4.7 mil, or 119 μm.

The same prepreg combination can therefore produce substantially different thickness estimates when the copper retention changes.

How Should This Formula Be Used?

This formula explains resin filling demand and supports an initial assessment. It does not replace stack-up validation by the PCB manufacturer.

Actual lamination also depends on resin flow, curing shrinkage, glass fabric support, local copper distribution, and the lamination cycle. A panel’s average copper retention cannot fully describe the filling demand in every local area.

A particularly important point is:

If a reference pressed thickness already accounts for a specific copper thickness and copper retention ratio, subtracting that filling demand again would double-count the adjustment.

The formula estimates the dielectric spacing defined above. It does not calculate the finished thickness of the entire PCB or the minimum insulation distance at every location.

Total PCB thickness requires a consistent accounting of cores, other prepreg layers, and copper layers, without counting any component twice.

8. What Should Customers Confirm When Selecting Prepreg?

For PCB buyers and designers, the most useful step is to obtain a complete stack-up from the manufacturer, rather than simply confirming how many plies of 1080 or 7628 will be used.

Four points deserve particular attention:

  1. Material compatibility
    The prepreg and cores should form a confirmed, compatible material combination that meets the project’s thermal and electrical requirements.
  2. Sufficient resin for filling
    Heavy copper, low copper retention, or large local differences in copper distribution require careful evaluation of resin filling capability.
  3. Dielectric thickness after lamination
    Impedance calculations should use the confirmed dielectric thickness, rather than glass fabric thickness or an unadjusted material reference value.
  4. Consistency in volume production
    Projects with sensitive thickness or impedance requirements should be validated through lamination trials, microsection measurements, and impedance testing where required.

In Multilayer PCB Manufacturing, prepreg selection connects the stack-up design with actual manufacturing capability. For High-Reliability PCBs, adequate resin filling and consistent interlayer insulation must also be addressed during stack-up planning.

9. Understanding Prepreg Requires More Than Remembering Glass Style Numbers

1080, 2116, and 7628 are only the starting point.

The final lamination result depends on the combined effects of glass style, resin system, resin content, prepreg combination, copper thickness, copper distribution, and processing conditions.

For customers, a reliable stack-up should explain which materials will be used, what dielectric thickness is expected, and how that result will be verified.

At SQPCB, we evaluate prepreg combinations against the customer’s copper patterns and board thickness requirements before production. Whether the project requires Quick-Turn PCB Manufacturing or volume production, a suitable material combination and a realistic pressed thickness are essential starting points.

Tony Niu | PCB Manufacturer | 25 Years of Industry Experience

Product Center
Contact Us

Get A Quote

kgr6iz
Quote
E-mail
info@sqpcb.com
Whatsapp
+86 136 0306 3656